GRADUAL LAB / MATERIALS

01 / Theory before the experiment

From a phase diagram
to a microstructure

Why does low-carbon steel contain ferrite and pearlite, while higher-carbon steel contains pearlite and cementite?

Explore the interactive lab →

1. Read a state, then follow a path

The horizontal axis is the alloy’s carbon content in weight percent. The vertical axis is temperature in °C. At a fixed overall composition, cooling follows a vertical line. Crossing a boundary changes which phases can coexist at equilibrium. A two-phase field does not mean each phase has the overall carbon content: each has its own composition at the ends of a horizontal tie line.

The liquidus marks where solid first appears on cooling. Below the solidus, solidification is complete. In steel, the A₃ and Acm boundaries mark the appearance of proeutectoid ferrite or cementite from austenite.

This is the metastable iron–cementite (Fe–Fe₃C) diagram. Cementite is retained instead of graphite. The lab assumes slow cooling and uses straight-line boundary approximations. It does not predict quenching, martensite, grain size, hardness values or real transformation times.

2. Phases and microconstituents

TermWhat it isStructure / composition
α ferriteOne solid phaseBCC iron; very little dissolved carbon
γ austeniteOne solid phaseFCC iron; greater carbon solubility
δ ferriteOne solid phaseHigh-temperature BCC iron
Fe₃C cementiteOne solid phaseOrthorhombic carbide; 6.67 wt% C
PearliteMicroconstituent with two phasesAlternating ferrite and cementite lamellae
LedeburiteEutectic microconstituentγ + Fe₃C as formed; γ transforms on further cooling

Proeutectoid means “formed before the eutectoid reaction.” Proeutectoid ferrite and ferrite inside pearlite are the same phase, but occupy different parts of the microstructure. The same distinction applies to proeutectoid cementite and cementite inside pearlite.

The unit-cell viewer counts shared atoms: BCC contains \(8(1/8)+1=2\) iron atoms per cell; FCC contains \(8(1/8)+6(1/2)=4\). Atom sizes are reduced to expose the arrangement; carbon occupancy is omitted.

3. Three steel cooling stories

Hypoeutectoid steel, below 0.76 wt% C: start in austenite, cross A₃, and form proeutectoid ferrite. Carbon partitions into the remaining austenite. At A₁, that austenite has the eutectoid composition and becomes pearlite.

Eutectoid steel, 0.76 wt% C: austenite becomes pearlite without first forming a separate proeutectoid constituent.

Hypereutectoid steel, above 0.76 and up to 2.11 wt% C: cross Acm and form proeutectoid cementite. At A₁, the remaining austenite becomes pearlite. The schematic draws the earlier cementite along grain boundaries.

\[\gamma\;\xrightarrow[\text{slow cooling}]{727\,{}^\circ\mathrm{C}}\;\alpha+\mathrm{Fe}_3\mathrm{C}\]

At 1147 °C and eutectic composition 4.30 wt% C, liquid forms γ + Fe₃C. At 1493 °C, liquid and δ react to form γ at the peritectic. At an invariant reaction, temperature and overall composition do not determine unique amounts of all three phases; the transformation’s progress is also needed.

What changes inside the remaining austenite?

As hypoeutectoid steel cools through the α + γ field, newly formed ferrite accepts very little carbon. The remaining γ becomes richer in carbon, approaching the eutectoid composition at A₁. In hypereutectoid steel, carbon-rich cementite forms along grain boundaries; the remaining γ becomes poorer in carbon and also approaches the eutectoid composition.

The carbon content of the whole specimen stays fixed during both paths. What changes is how carbon is distributed among the coexisting phases. The lab’s carbon-partition readout reports the γ endpoint of the current tie line.

At approximately 01:20–02:05, Part II compares solidification and solid-state decomposition using analogous diagram shapes. Their starting states differ: solidification starts with melt, while the eutectoid reaction starts with solid austenite. A₃ and Acm are solid-state boundaries, not extra liquidus lines.

4. The lever rule is a carbon balance

Let \(C_0\) be the overall composition, and \(C_L,C_R\) the carbon contents of the two coexisting phases. Their mass fractions satisfy

\[w_L+w_R=1,\qquad C_0=w_LC_L+w_RC_R.\]

Solving these two balances gives the opposite-arm rule:

\[w_L=\frac{C_R-C_0}{C_R-C_L},\qquad w_R=\frac{C_0-C_L}{C_R-C_L}.\]

These are mass fractions because the axis uses weight percent. A schematic grain area is not a measured mass fraction. The lab reports numerical fractions separately from its illustrative drawing.

5. Worked example: 0.30 wt% C steel

To find proeutectoid ferrite and pearlite, take the tie line just above 727 °C: ferrite contains 0.022 wt% C and the remaining austenite contains 0.76 wt% C. That austenite becomes pearlite just below A₁.

\[w_P=w_\gamma=\frac{0.30-0.022}{0.76-0.022}=0.3767,\qquad w_{\alpha,\mathrm{pro}}=1-w_P=0.6233.\]

The result is approximately 37.7% pearlite and 62.3% proeutectoid ferrite by mass. This does not mean 37.7% cementite. To find total cementite just below A₁, use the ferrite–cementite endpoints instead:

\[w_{\mathrm{Fe}_3\mathrm{C}}=\frac{0.30-0.022}{6.67-0.022}=0.04182\approx4.18\%.\]

For 1.40 wt% C steel, the pearlite fraction is \((6.67-1.40)/(6.67-0.76)\approx89.2\%\), leaving 10.8% proeutectoid cementite. Total cementite also includes the cementite inside pearlite.

Below A₁, the lab keeps the microconstituent split calculated at 727 °C. The current phase fractions separately use an approximate ferrite solubility that decreases from 0.022 wt% C at 727 °C to 0.008 wt% C at 400 °C. Small later precipitation is omitted from the grain morphology.

6. Read the cooling curve alongside the diagram

The phase diagram shows temperature versus composition. A cooling curve instead shows temperature versus time for one fixed composition. As cooling proceeds, the markers on both plots show the same temperature.

When a transformation releases latent heat, it can slow the temperature drop. An ideal equilibrium invariant transformation appears as a horizontal thermal arrest. In this lab the eutectoid arrest is at 727 °C; the relevant cast-iron paths also show a eutectic arrest at 1147 °C. Pure iron has separate arrests at solidification and its crystal-structure changes.

Press Cool alloy to trace the curve. During a hold the curve marker moves horizontally while the phase-diagram marker stays at the reaction temperature. Pause, scrub the curve, change the speed or reset to explore the same path. A thermal arrest does not by itself fix unique three-phase amounts.

The horizontal axis is relative time. Slopes and hold widths are illustrative; a phase diagram alone cannot supply a measured cooling history or transformation duration.

The videos use rounded values such as 0.8 wt% C, 723 °C and 2.06 wt% C; the original explorer uses 0.76 wt% C, 727 °C and 2.11 wt% C. Those conventions produce slightly different percentages. This lab consistently retains the explorer’s values. The steel/cast-iron division here is a diagram convention, not a claim that every commercial alloy is classified by carbon content alone.

For further reading: H. K. D. H. Bhadeshia’s Interpretation of steel microstructure explains the phases, cooperative pearlite growth and the role of transformation mechanisms. Aalto University’s Fe–C phase-diagram lesson develops tie-line and lever-rule balances; its rounding convention differs.

Microconstituent fractions across the steel range

Part II’s final chart (around 20:05) shows pearlite increasing to the eutectoid composition, then decreasing as proeutectoid cementite increases. The interactive chart reproduces that relationship using this lab’s 0.76 wt% C convention and A₁ mass balances. At 0.30 wt% C, it gives 37.7% pearlite; at 0.76 wt% C, 100%; at 1.40 wt% C, 89.2%. The chart describes the mixture just after the eutectoid transformation; it does not claim that mass fractions equal visible grain areas.

Try it yourself

  1. Cool 0.30 wt% C steel from 950 °C. What appears before pearlite?
  2. At 700 °C, compare “Current phases” with “Pearlite split.” Explain why the two percentages differ.
  3. Repeat for 1.40 wt% C. Which proeutectoid phase changes?
  4. Select exactly 727 °C. Why does the lab withhold unique phase fractions?
Test your predictions in the lab →